US0087.09611B2
`
`(12) United States Patent
`Haley
`
`(10) Patent No.:
`(45) Date of Patent:
`
`US 8,709,611 B2
`Apr. 29, 2014
`
`(54) MULTILAYER FILMS HAVING REDUCED
`CURLING
`
`(75) Inventor: Jeffrey C. Haley, Cincinnati, OH (US)
`(73) Assignee: Fightar Chemicals, LP, Houston, TX
`
`(*) Notice:
`
`Subject to any disclaimer, the term of this
`patent is extended or adjusted under 35
`U.S.C. 154(b) by 204 days.
`
`(21) Appl. No.: 12/802,523
`
`(22) Filed:
`
`Jun. 8, 2010
`
`(65)
`
`Prior Publication Data
`US 2011 FO3OO391 A1
`Dec. 8, 2011
`(51) Int. Cl.
`B32B 27/08
`(2006.01)
`B32B 27/00
`(2006.01)
`B32B 27/30
`(2006.01)
`B32B 27/32
`(2006.01)
`B29C 65/00
`(2006.01)
`(52) U.S. Cl.
`USPC ..................... 428/516; 428/4744; 428/476.9;
`428/522; 428/523: 156/60
`(58) Field of Classification Search
`None
`See application file for complete search history.
`
`(56)
`
`References Cited
`
`U.S. PATENT DOCUMENTS
`
`4/2004 Botros
`6,716,928 B2
`7,569,630 B2 * 8/2009 Ma et al. ....................... 524,221
`2004/OO38055 A1
`2/2004 Hawighorst
`2008/0227900 A1* 9, 2008 Borke et al. .................. 524,388
`2009/00291.82 A1
`1/2009 Aubee et al. ............... 428,476.9
`OTHER PUBLICATIONS
`Barry A. Morris, DuPont, Wilmington, Delaware, “Reducing Curlin
`Multilayer Blown Film. Part I: Experimental Results, Model Devel
`opment and Strategies.” Presented at 2001 TAPPI Polymers, Lami
`nations and Coatings Conference, Aug. 27-30, 2001.
`Barry A. Morris, DuPont, Wilmington, Delaware, “Reducing Curlin
`Multilayer Blown Film. Part II: Application of Predictive Modeling
`to a Barrier Cereal Liner Film.” Presented at 2001 TAPPI Polymers,
`Laminations and Coatings Conference, Aug. 27-30, 2001.
`PCT International Search Report and the Written Opinion—Mailed
`Nov. 21, 2011 for Corresponding PCT/IB2011/00 1680.
`* cited by examiner
`
`Primary Examiner — Sheeba Ahmed
`
`(57)
`ABSTRACT
`Disclosed is a multilayer film. The multilayer film has the
`general structure of A/B/A/C or B/A/B/C, wherein A is a
`nucleated high density polyethylene (HDPE) layer. B is a
`single or multilayer structure, and C is a seal layer. Adding a
`nucleating agent to HDPE improves the water vapor barrier
`property of the HDPE layer and the multilayer film, but it also
`causes the multilayer film to curl in the conventional multi
`layer film structures. The invention provides a multilayer
`film, which includes at least one layer of nucleated HDPE,
`with reduced or eliminated curling while retaining high water
`vapor barrier.
`
`4,906,172 A *
`6,306,996 B1
`
`3, 1990 Stewart ...................... 425, 1744
`10, 2001 Cecchin et al.
`
`15 Claims, No Drawings
`
`EPL LIMITED EX1006
`U.S. Patent No. 10,889,093
`
`0001
`
`

`

`1.
`MULTILAYER FILMS HAVING REDUCED
`CURLING
`
`US 8,709,611 B2
`
`FIELD OF THE INVENTION
`
`The invention relates to a multilayer film. More particu
`larly, the invention relates to a multilayer film that possesses
`good water vapor barrier property and reduced curling.
`
`BACKGROUND OF THE INVENTION
`
`10
`
`15
`
`Polyethylene is widely used to prepare food packaging
`films and bags such as cereal liners and cake mix bags, gro
`cery bags, stretch-wraps, shrink-wraps, garbage can liners,
`and shipping bags. Some applications, such as food packag
`ing films and bags, require films to have sufficient water vapor
`and oxygen barrier properties to preserve the contents. The
`packaging films usually have a multilayer structure. Depend
`ing on the intended application, the number, type, and
`arrangement of layers employed will vary. Ethylene-vinyl
`alcohol (EVOH) copolymers and polyamides (nylons) are
`often used as barrier layers. Polyethylene is often used as one
`or more layers.
`High density polyethylene (HDPE) is often used as a layer
`in the multilayer films because of its high strength and modu
`25
`lus. HDPE can be nucleated. Nucleated HDPE has improved
`water vapor barrier property. Thus when nucleated HDPE is
`used as a layer in a multilayer film, it provides the film not
`only with physical strength but also with increased barrier to
`water vapor. One problem associated with the use of nucle
`ated HDPE in a multilayer film is that nucleated HDPE causes
`the multilayer films to curl to a greater extent. The curling
`brings inconvenience to the film manufacturers and consum
`ers. Therefore, there is a need to reduce or eliminate the
`curling of multilayer film caused by the use of nucleated
`HDPE.
`
`30
`
`35
`
`SUMMARY OF THE INVENTION
`
`45
`
`The invention relates to a multilayer film. By “film. I mean
`40
`to include both films (which are normally referred to those
`having a thickness less than or equal to 10 mils) and sheets
`(which are normally referred to those having a thickness
`greater than 10 mils). The multilayer film of the invention has
`the general structure of A/B/A/C or B/A/B/C, wherein A is a
`nucleated high density polyethylene (HDPE) layer, B is a
`single or multilayer structure, and C is a seal layer. Preferably
`the seal layer C is selected from the group consisting of linear
`low density polyethylenes (LLDPE), low density polyethyl
`enes (LDPE), ethylene-vinyl acetate copolymers (EVA),
`polyolefin ionomers, the like, and mixtures thereof. Adding a
`nucleating agent to HDPE improves the water vapor barrier
`property of the HDPE layer and the multilayer film thereby.
`However, nucleated HDPE causes the multilayer film to curl
`to a greater extent in the conventional multilayer film struc
`tures. The invention provides a multilayer film, which
`includes at least one layer of nucleated HDPE, with reduced
`or eliminated curling while retaining high water vapor barrier.
`
`50
`
`55
`
`DETAILED DESCRIPTION OF THE INVENTION
`
`60
`
`The invention is a multilayer film. The multilayer film has
`the general structure of A/B/A/C or B/A/B/C, wherein A is a
`nucleated high density polyethylene (HDPE) layer, B is a
`single or multilayer structure, and C is a seal layer. By “nucle
`ated HDPE, I mean that the HDPE contains a nucleating
`agent. Unless specified as “nucleated HDPE in this appli
`
`65
`
`2
`cation, the term HDPE refers only to those which do not
`contain nucleating agents. By 'seal layer.' I mean the layer of
`the multilayer film which softens at lower temperature than
`the rest layers of the film structure, so that the film can be heat
`sealed. Seal layer may directly contact with the goods, such as
`meat or vegetables, protected by the multilayer film.
`Suitable nucleated HDPE comprises a nucleating agent
`and an HDPE resin. Suitable HDPE for making the nucleated
`HDPE includes ethylene homopolymers and copolymers of
`ethylene and C-olefins. Suitable O.-olefins include 1-butene,
`1-hexene, and 1-octene, the like, and mixtures thereof. Pref
`erably, the C-olefin content in the nucleated HDPE is less than
`2 wt %. The nucleated HDPE has a density preferably within
`the range of 0.940 to 0.970 g/cm, and more preferably within
`the range of 0.945 to 0.965 g/cm. The nucleated HDPE has
`a melt index MI preferably within the range of 0.001 to 100
`dg/min, and more preferably within the range of 0.05 to 50
`dg/min. Density is measured according to ASTM D1505; and
`MI is measured according to ASTM D 1238 at 190° C. and
`2.16 kg. Unless specifically mentioned, all density and MI in
`this application are measured according to these ASTM meth
`ods.
`The nucleated HDPE can be multimodal. By “multimo
`dal. I mean that the nucleated HDPE comprises at least two
`components, one of which has a relatively low molecular
`weight, and the other which has a relatively high molecular
`weight. Many HDPE resins are commercially available; for
`instance L5885 and M6020 HDPE are resins from Equistar
`Chemicals, LP. They can be readily nucleated by a nucleating
`agent.
`Suitable nucleating agents for making the nucleated HDPE
`include those known to the industry. Preferably, the nucleat
`ing agents are selected from the group consisting of glycerol
`alkoxide salts, hexahydrophthalic acid salts, the like, and
`mixtures thereof. The salts include ammonium and metal
`salts. Preferably, the glycerol alkoxide salt is selected from
`the group consisting of Zinc, magnesium, and calcium glyc
`erolates and mixtures thereof. More preferably, the glycerol
`alkoxide salt is a zinc glycerolate. Preferably, the hexahydro
`phthalic acid salt is selected from the group consisting of zinc,
`magnesium, and calcium hexahydrophthalates, the like, and
`mixtures thereof. More preferably, the hexahydrophthalic
`acid salt is calcium hexahydrophthalate. Many glycerol
`alkoxide salts and hexahydrophthalic acid salts are commer
`cially available. For instance, Zinc glycerolate is available
`from Ciba Specialty Chemicals as Irgastab(R) 287. Calcium
`hexahydrophthalate is available from Milliken Company as
`Hyperform(RHPN-20E. The amount of nucleating agent used
`in the nucleated HDPE varies depending on many factors
`such as the nucleating agent type, the properties of the HDPE,
`and the targeted improvement of the barrier properties. In
`general, the nucleating agent is used in an amount within the
`range of 0.01 to 1 wt % of the HDPE. Preferably, the amount
`of the nucleating agent is within the range of 0.05 to 0.5 wt %
`of the HDPE.
`The seal layer C is preferably selected from the group
`consisting of linear low density polyethylene (LLDPE), low
`density polyethylene (LDPE), ethylene-vinyl acetate copoly
`mers (EVA), polyolefin ionomers, the like, and mixtures
`thereof. Suitable LLDPE resins include copolymers of ethyl
`ene and C-olefins. Suitable C-olefins include 1-butene, 1-hex
`ene, and 1-octene, the like, and mixtures thereof. The C-olefin
`content in the LLPDE is preferably within the range of 5 to 15
`wt %. The LLDPE has a density preferably within the range of
`0.865 to 0.935 g/cm, and more preferably within the range
`0.905 to 0.935 g/cm. The LLDPE has a melt index MI
`preferably within the range of 0.5 to 50 dg/min, and more
`
`0002
`
`

`

`US 8,709,611 B2
`
`10
`
`15
`
`30
`
`35
`
`40
`
`3
`preferably within the range of 1 to 15 dg/min. Many LLDPE
`resins are commercially available; for instance GS707
`LLDPE and GA501 are from Equistar Chemicals, LP.
`Suitable LDPE for use in the invention include those
`known to the industry. LDPE is usually made by free radical
`polymerization under high pressure. There are two basic pro
`cesses for the manufacture of LDPE: autoclave and tubular.
`Both autoclave LDPE and tubular LDPE are Suitable for use
`in the invention. The LDPE has a density preferably within
`the range of 0.915 to 0.935 g/cm, and more preferably within
`the range of 0.918 to 0.932 g/cm. The LDPE has a melt index
`MI preferably within the range of 0.1 to 100 dg/min, and
`more preferably within the range of 0.5 to 50 dg/min. Many
`LDPE resins are commercially available and suitable for use
`as a seal layer. An example of suitable LDPE resin is Petroth
`ene NA860 from Equistar Chemicals, LP. Ethylene-vinyl
`acetate copolymers (EVA) are made by the free radical copo
`lymerization of ethylene and vinyl acetate. Suitable EVA
`comprises preferably from 2 to 30 wt % of vinyl acetate, and
`more preferably from 5 to 18 wt % of vinyl acetate. The
`suitable EVA has a melt index MI preferably within the range
`of 2 to 500 dg/min. Many EVA resins are commercially
`available; for instance, EVA UE624 is a product of Equistar
`Chemicals, LP. Suitable polyolefin ionomers include ammo
`25
`nium and metal salts of olefin-acrylic acid and olefin-meth
`acrylic acid copolymers. Examples are sodium, Zinc, and
`magnesium salts of ethylene-acrylic acid copolymers and
`ethylene-methacrylic acid copolymers. Many polyolefin
`ionomers are commercially available; for instance, the Sur
`lyn Rionomers is from Du Pont Chemical Company.
`Layer B can be a single layer or a multilayer structure.
`When B is a single layer, it is preferably a polyolefin layer.
`Suitable polyolefin for use as a Blayer in the multilayer film
`of the invention is preferably selected from the group consist
`ing of polyethylene, polypropylene, and poly 1-butene. Suit
`able polyethylene include the above-discussed HDPE,
`LLDPE, and LDPE, the like, and mixtures. Suitable polypro
`pylene includes amorphous polypropylene, semi-crystalline
`polypropylene, the like, and mixtures thereof. Preferably, the
`semi-crystalline polypropylene is selected from the group
`consisting of propylene homopolymers, copolymers of pro
`pylene with at least one other C to Co C-olefin, the like, and
`mixtures thereof. Copolymers of propylene include random
`copolymers and impact copolymers. Preferred C-olefins for
`Such copolymers include ethylene, 1-butene, 1-pentene,
`1-hexene, methyl-1-butenes, methyl-1-pentenes, 1-octene,
`1-decene, the like, and mixtures thereof. “Semi-crystalline.”
`as used herein, means that the crystallinity is greater than or
`equal to 40%, preferably greater than or equal to 55%, and
`more preferably greater than or equal to 80%. Preferably, the
`semi-crystalline polypropylene has a melt flow rate (as deter
`mined by ASTM D-1238-01 at a temperature of 230° C. and
`at a load of 2.16 kg) within the range of 0.001 to 500 dg/min.
`Preferably, the semi-crystalline polypropylene has a density
`within the range of 0.897 to 0.925 g/cm and a weight average
`molecular weight (Mw) within the range of 85,000 to 900,
`000. Suitable poly 1-butene includes homopolymers of
`1-butene, copolymers of 1-butene with at least one other C to
`Co C-olefin, the like, and mixtures thereof. Preferred C-ole
`fins for Such copolymers include ethylene, propylene, 1-pen
`tene, 1-hexene, methyl-1-butenes, methyl-1-pentenes,
`1-octene, 1-decene, the like, and mixtures thereof. The poly 1
`butene has a melt index preferably within the range of 0.01 to
`1000 dg/min, more preferably within the range of 0.1 to 750
`dg/min. Methods for producing poly 1-butene are known. For
`instance, see U.S. Pat. No. 6,306,996; the teachings of this
`
`55
`
`45
`
`50
`
`60
`
`65
`
`4
`patent are herein incorporated by reference. Polyethylene is a
`preferred polyolefin for use as a B layer. HDPE and LLDPE
`are particularly preferred.
`When Blayer is a multilayer structure, B preferably has a
`structure of tie layer/barrier layer/tie layer and the multilayer
`film preferably has a structure of A/B/NC. Tie layer is also
`called tie layer adhesive or adhesive layer. Preferably the tie
`layer resin comprises a maleated polyolefin. It comprises
`preferably from 0.5 to 25 wt %, preferably 5 to 20 wt %, and
`more preferably 5 to 15 wt %, of a maleated polyolefin.
`Suitable maleated polyolefin for use as a tie layer in the
`invention include maleated polyethylene, maleated polypro
`pylene, and maleated poly 1-butene. Methods for maleating
`polyolefin are known. For instance, U.S. Pat. No. 6,716,928,
`the teachings of which are incorporated herein by reference,
`teaches maleating a propylene impact copolymer. Suitable
`polyethylene, polypropylene, and poly 1-butene for making
`the maleated polyolefin include those discussed above. Pref
`erably, the maleated polyolefin is a maleated HDPE. The
`maleated polyolefin contains preferably from 0.1 to 10 wt %,
`more preferably from 0.5 to 5 wt %, and most preferably from
`1 to 2.5 wt %, of grafted maleic anhydride. Preferably the tie
`layer resin comprises an elastomer. Suitable elastomers
`include olefin-based elastomers and conjugated diene-based
`elastomers. By “olefin elastomer.' I mean any olefin poly
`mers or copolymers which have elastomeric characteristics.
`Suitable polyolefin elastomers include ethylene-propylene
`rubber, ethylene-acrylate rubber, ethylene-1-butene rubber,
`ethylene-propylene-diene rubber (EPDM), polyethylene
`plastomers, elastoplastic polypropylene or impact polypro
`pylene, the like, and mixtures thereof. Preferably the poly
`olefinelastomers are selected from the group consisting of
`ethylene-propylene rubber, ethylene-1-butene rubber,
`EPDM, the like, and mixtures thereof. Ethylene-propylene
`rubber is particularly preferred. By "conjugated diene-based
`elastomer.' I mean any conjugated diene-containing poly
`mers and copolymers which have a glass transition tempera
`ture (T) below room temperature (25° C.). In other words,
`the conjugated diene-containing polymers and copolymers
`are in elastomeric or rubber state at room temperature.
`Examples of conjugated diene-based elastomers include
`polybutadiene, polyisoprene, butadiene-vinyl aromatic ran
`dom and block copolymers, isoprene-vinyl aromatic random
`and block copolymers, hydrogenated butadiene-vinyl aro
`matic block copolymers, hydrogenated isoprene-vinyl aro
`matic block copolymers, the like, and mixtures thereof. Pref
`erably, the conjugated diene-based elastomers are selected
`from the group consisting ofbutadiene-styrene block copoly
`mers, isoprene-styrene block copolymers, hydrogenated
`butadiene-styrene block copolymers, hydrogenated isoprene
`styrene block copolymers, the like, and mixture thereof. More
`preferably, the conjugated diene-based elastomers are
`selected from the group consisting of styrene-butadiene-sty
`rene triblock copolymers (SBS), styrene-isoprene-styrene tri
`block copolymers (SIS), the like, and mixtures thereof. SBS
`is particularly preferred. The tie layer resin comprises pref
`erably from 15 to 65 wt %, more preferably from 25 to 55 wt
`%, and most preferably from 25 to 45 wt %, of the elastomer.
`The tie layer resin preferably comprises a base resin in an
`amount within the range of 35 to 95 wt % of the tie layer resin.
`LLDPE is a preferred based resin for the tie layer. Suitable
`LLDPE includes those which are discussed above.
`Suitable barrier layer includes any polymers which provide
`water vapor or oxygen barrier properties. Suitable barrier
`layer is preferably selected from the group consisting of eth
`ylene-vinyl alcohol copolymers (EVOH), polyamides (ny
`lons), the like, and mixture thereof. Suitable polyamides
`
`0003
`
`

`

`US 8,709,611 B2
`
`6
`With these two dimensions, the radius of curvature, r, is
`calculated numerically using the equation
`
`5
`include nylon 6, nylon 6.6, nylon 12, nylon 6.12, nylon 6.66,
`the like, and mixtures thereof. EVOH is made by saponifica
`tion/hydrolysis of EVA. Suitable EVOH contains preferably
`from 30 to 50 molar % of vinyl alcohol.
`The multilayer film of the invention can be made by a
`variety of processes. It can be made by co-extrusion, coating,
`and other laminating processes. The film can be made by
`casting or blown film processes. Blown film processes
`include high-stalk and in-pocket processes. In a high-stalk
`process, the extrudate exits the annular opening in the die in
`the form of a tubular “stalk’ that is inflated a distance (usually
`the length of the stalk) from the extrusion die. For an in
`pocket blown process, the tube is inflated as the tube exits the
`extrusion die. After the tube is flattened and cooled, it can be
`slit to form a film.
`The invention includes a method for reducing or eliminat
`ing the curling of a multilayer film having the general struc
`ture of A/B/C. The method comprises adding a layer to the
`multilayer film to form a new film structure of A/B/NC or
`B/A/B/C. Layers A, B, and C are discussed above.
`The multilayer thin film of the invention has many uses. It
`is particularly useful for food packaging films and bags where
`low curling and low water vapor permeation rate are required,
`including cereal liners and cake mix bags.
`The following examples merely illustrate the invention.
`Those skilled in the art will recognize many variations that are
`within the spirit of the invention and scope of the claims.
`Comparative Example 1
`
`A three-layer film, A/B/C, is produced using a blown film
`line capable of producing films with up to seven layers. The
`film is produced at a rate of 2001b/hr, using a 0.095 inch thick
`die gap, a frost line height of 15 inches, and a blow up ratio of
`2.5:1. The film is 0.002 inch thick. Resins A and C are the
`outer layers of the film and Resin B is the center layer of the
`film. Resin A is a nucleated HDPE. The HDPE is an ethylene
`homopolymer having a density of 0.960 g/cm and a melt
`index MI of 2.0 dg/min. Resin A contains 500 ppm of a
`nucleating agent (Hyperform(R) HPN-20E is from Milliken
`and Company). The nucleating agent is used to improve the
`water vapor barrier properties of the film. Resin B is an HDPE
`copolymer with a density of 0.947 g/cm and MI of 1.1
`dg/min. Resin C is an LDPE with a density of 0.920 g/cm and
`a MI of 1.0 dg/min. The percentage of the total film taken by
`each layer in the A/B/C film structure is 35%/50%/15%.
`Film curling is characterized by cutting a 2 inchx2 inch
`“X” into each film, where the two cuts of the X are perpen
`dicular. Each cut is oriented with a 45 degree angle to both the
`machine and transverse directions. The two cuts produce four
`triangles, which are then free to curl. The X is oriented so that
`two of the triangles curl only in the machine direction of the
`film, and two of the triangles curled only in the transverse
`direction. The films are mounted onto a rigid Substrate and
`allowed to curl for 20 hours. After 20 hours, the direction of
`curl (either towards or away from the side of the film with
`resin C) is noted, and the radii of curvature of the curl in both
`the machine and transverse directions are measured. A larger
`radius of curvature in this measurement indicates less curl.
`When films curl by an amount that is more than 90 degrees,
`the radius of curvature is measured directly. When films curl
`less than 90 degrees, it is difficult to measure the radius
`directly. In these cases, the radius of curvature is determined
`by measuring the distance, 1, from the base of the triangle to
`its free point and the distance, w, from the base of the triangle
`to the projection of the free point into the plane of the film.
`
`5
`
`10
`
`15
`
`25
`
`30
`
`35
`
`40
`
`45
`
`50
`
`55
`
`60
`
`65
`
`The curl direction and radius of curvature in the machine
`(MD) and transverse (TD) directions of this film are tabulated
`in Table 1. Comparative Example 1 shows a very large ten
`dency to curl, as indicated by its very small radius of curvature
`in both of the machine and transverse directions. This film
`curls towards the C layer direction. Water vapor transmission
`rate is measured at 100% relative humidity following the
`method of ASTM F1249. The 1% secant modulus in the
`machine direction is measured following the method of
`ASTM E111. Water vapor transmission rate and modulus are
`tabulated in Table 1.
`
`Example 2
`
`A four-layer film is produced using the same film equip
`ment and processing conditions as used in Comparative
`Example 1. This film has the same total thickness as the film
`in Comparative Example 1 (0.002 in). Identical resins A, B
`and C are used to produce this film structure. The four layer
`structure is arranged as an A/B/NC film, where the percentage
`of the total film in each layer is 7%/50%/28%/15%. The total
`fraction of the film taken up by the combined Alayers is 35%,
`which is identical to the A fraction in Comparative Example
`1. Curl testing is performed on Example 2 in a manner iden
`tical to the test used on Comparative Example 1, and the
`results are presented in Table 1. Example 2 curls away from
`the C layer direction (the direction opposite of the curl direc
`tion of Comparative example 1). Example 2 curls less than
`Comparative Example 1, as indicated by the much higher
`radii of curvature. Water vapor transmission rate is measured
`at 100% relative humidity following the method of ASTM
`F1249. The 1% secant modulus in the machine direction is
`measured following the method of ASTM E111. Water vapor
`transmission rate and modulus are tabulated in Table 1. The
`water vaportransmission rate and modulus are essentially the
`same as Comparative Example 1.
`Example 3
`
`A four-layer film is produced using the same film equip
`ment and processing conditions as used in Comparative
`Example 1. This film has the same thickness as the film in
`Comparative Example 1 (0.002 in). Identical resins A, B and
`C are used to produce this film structure. The four-layer
`structure is arranged as an A/B/A/C film, where the percent
`age of the total film in each layer was 15%/50%/20%/15%.
`The total fraction of the film taken up by the combined A
`layers is 35%, which is identical to the A fraction in Com
`parative Example 1. Curl testing is performed on Example 3
`in a manner identical to the test used on Comparative
`Example 1, and the results are presented in Table 1. Example
`3 curls toward the C layer direction (the same direction as the
`curl direction of Comparative Example 1, and the opposite
`direction as the curl direction in Example 2). Example 3 curls
`less than Comparative Example 1, as indicated by the much
`higher radii of curvature. Water vapor transmission rate is
`measured at 100% relative humidity following the method of
`ASTM F1249. The 1% secant modulus in the machine direc
`tion was measured following the method of ASTM E111.
`
`0004
`
`

`

`7
`Water vapor transmission rate and modulus are tabulated in
`Table 1. The water vapor transmission rate and modulus are
`essentially the same as Comparative Example 1.
`Comparative Example 4
`
`A three-layer film is produced using the same film equip
`ment and processing conditions as used in Comparative
`Example 1. This film has the same thickness as Comparative
`Example 1 (0.002 in). Resins B and C are the same materials
`that are used in Comparative Example 1. Resin A is an HDPE
`homopolymer with a density of 0.960 g/cm and a MI of 1.1
`dg/min. Resin A contains 500 ppm of a nucleating agent
`(Hyperform R) HPN-20E is from Milliken and Company)
`used to improve the water vapor barrier properties of the film.
`The three-layer film structure is arranged as a B/A/C film
`structure, where percentage of the total film taken by each
`layer is 35%/50%/15%. Curl testing is performed on Com
`parative Example 4 in a manner identical to the test used on
`Comparative Example 1, and the results are presented in
`Table 1. Comparative Example 4 curls away from the C layer
`direction. Water vapor transmission rates are measured at
`100% relative humidity following the method of ASTM
`F1249. The 1% secant modulus in the machine direction is
`measured following the method of ASTM E111. Water vapor
`transmission rate and modulus are tabulated in Table 1.
`
`10
`
`15
`
`25
`
`Example 5
`
`30
`
`35
`
`40
`
`A four-layer film is produced using the same film equip
`ment and processing conditions as used in Comparative
`Example 4. This film has the same thickness as the film in
`Comparative Example 4 (0.002 in). Identical resins A, B and
`C are used to produce this film structure. The four-layer
`structure is arranged as a B/A/B/C film, where the percentage
`of the total film in each layer was 20%/50%/15%/15%. The
`total fraction of the film taken up by the combined Blayers is
`35%, which is identical to the B fraction in Comparative
`Example 4. Curl testing is performed on Example 5 in a
`manner identical to the test used on Comparative Example 1,
`and the results are presented in Table 1. Example 5 curls
`toward the C layer direction (the direction opposite of the curl
`direction of Comparative example 4). Example 5 curls less
`than Comparative Example 4, as indicated by the higher radii
`of curvature. Water vapor transmission rate is measured at
`45
`100% relative humidity following the method of ASTM
`F1249. The 1% secant modulus in the machine direction is
`measured following the method of ASTM E111. Water vapor
`transmission rate and modulus are tabulated in Table 1. The
`water vapor transmission rate and modulus are essentially the
`same as Comparative Example 4.
`Example 6
`
`50
`
`A four-layer film is produced using the same film equip
`ment and processing conditions as used in Comparative
`Example 4. This film has the same thickness as the film in
`Comparative Example 4 (0.002 in). Identical resins A, B and
`C are used to produce this film structure. The four-layer
`structure is arranged as a B/NB/C film, where the percentage
`of the total film in each layer was 25%/50%/10%/15%. The
`total fraction of the film taken up by the combined Blayers is
`35%, which is identical to the B fraction in Comparative
`Example 4. Curl testing is performed on Example 6 in a
`manner identical to the test used on Comparative Example 1,
`and the results are presented in Table 1. Example 6 essentially
`does not curl at all. Water vaportransmission rate is measured
`
`55
`
`60
`
`65
`
`US 8,709,611 B2
`
`8
`at 100% relative humidity following the method of ASTM
`F1249. The 1% secant modulus in the machine direction is
`measured following the method of ASTM E111. Water vapor
`transmission rate and modulus are tabulated in Table 1. The
`water vaportransmission rate and modulus are essentially the
`same as Comparative Example 4.
`
`TABLE 1
`
`RESULTS SUMMARY
`
`Ex. No.
`
`1% Secant
`MD Curvature TD Curvature WVTR
`Radius, mm Radius, mm g/m/day Modulus, kpsi
`
`C1
`2
`3
`C4
`5
`6
`
`3
`10
`14
`7
`9
`No Curl
`
`5
`12
`34
`2O
`25
`No Curl
`
`2.0
`2.0
`2.1
`2.0
`2.0
`2.0
`
`114
`114
`116
`117
`117
`119
`
`I claim:
`1. A multilayer film having a general structure of A/B/A/C
`or B/A/B/C, wherein A is a nucleated high density polyeth
`ylene (HDPE) layer, B is a single or multilayer structure, and
`C is a seal layer
`wherein the nucleated HDPE comprises an HDPE and a
`nucleating agent selected from the group consisting of
`glycerol alkoxide salts, hexahydrophthalic acid salts,
`and mixtures thereof
`wherein when the multilayer film has the structure A/B/A/
`C, A is present in a total amount equal to about 35 wt.%.
`based upon the total weight of the multilayer film, and
`wherein when the multilayer film has the structure B/A/
`B/C, B is present in a total amount equal to about 35 wt.
`%, based upon the total weight of the multilayer film.
`2. The multilayer film of claim 1, wherein C is selected
`from the group consisting of linear low density polyethylene
`(LLDPE), low density polyethylene (LDPE), ethylene-vinyl
`acetate copolymers (EVA), polyolefin ionomers, and mix
`tures thereof.
`3. The multilayer film of claim 1, wherein B is a single
`HDPE layer or LLDPE layer.
`4. The multilayer film of claim 1, having the general struc
`ture of A/B/A/C.
`5. The multilayer film of claim 4, wherein B is a multilayer
`structure of tie layer/barrier layer/tie layer.
`6. The multilayer film of claim 5, wherein the barrier layer
`is an ethylene-vinyl alcohol copolymer layer or a polyamide
`layer.
`7. The multilayer film of claim 5, wherein the tie layer
`comprises a maleated polyolefin.
`8. A method for reducing or eliminating the curling of a
`multilayer film having a general structure of A/B/C or B/A/C,
`said method comprising adding a layer to the multilayer film
`to form a new film structure of A/B/A/C or B/A/B/C; wherein
`A is a nucleated high density polyethylene (HDPE) layer, Bis
`a single or multilayer structure, and C is a seal layer
`wherein the nucleated HDPE comprises an HDPE and a
`nucleating agent selected from the group consisting of
`glycerol alkoxide salts, hexahydrophthalic acid salts,
`and mixtures thereof
`wherein when the multilayer film has the structure A/B/A/
`C, A is present in a total amount equal to about 35 wt.%.
`based upon the total weight of the multilayer film, and
`wherein when the multilayer film has the structure B/A/B/
`C, B is present in a total amount equal to about 35 wt.%.
`based upon the total weight of the multilayer film.
`
`0005
`
`

`

`US 8,709,611 B2
`
`10
`
`9
`9. The method of claim 8, wherein C is selected from the
`group consisting of LLDPE, LDPE, EVA, polyolefin iono
`mers, and mixtures thereof.
`10. The method of claim 8, wherein B is a single HDPE
`layer or LLDPE layer.
`11. The method of claim 10, wherein the new film structure
`is A/B/A/C.
`12. The method of claim 11, wherein B is a multilayer
`structure of tie layer/barrier layer/tie layer.
`13. The method of claim 12, wherein the barrier layer is an
`ethylene-Vinyl alcohol copolymer layer or a polyamide layer.
`14. The method of claim 12, wherein the tie layer com
`prises a maleated polyolefin.
`15. An article which comprises the multilayer film of claim
`
`1.
`
`10
`
`15
`
`0006
`
`

This document is available on Docket Alarm but you must sign up to view it.


Or .

Accessing this document will incur an additional charge of $.

After purchase, you can access this document again without charge.

Accept $ Charge
throbber

Still Working On It

This document is taking longer than usual to download. This can happen if we need to contact the court directly to obtain the document and their servers are running slowly.

Give it another minute or two to complete, and then try the refresh button.

throbber

A few More Minutes ... Still Working

It can take up to 5 minutes for us to download a document if the court servers are running slowly.

Thank you for your continued patience.

This document could not be displayed.

We could not find this document within its docket. Please go back to the docket page and check the link. If that does not work, go back to the docket and refresh it to pull the newest information.

Your account does not support viewing this document.

You need a Paid Account to view this document. Click here to change your account type.

Your account does not support viewing this document.

Set your membership status to view this document.

With a Docket Alarm membership, you'll get a whole lot more, including:

  • Up-to-date information for this case.
  • Email alerts whenever there is an update.
  • Full text search for other cases.
  • Get email alerts whenever a new case matches your search.

Become a Member

One Moment Please

The filing “” is large (MB) and is being downloaded.

Please refresh this page in a few minutes to see if the filing has been downloaded. The filing will also be emailed to you when the download completes.

Your document is on its way!

If you do not receive the document in five minutes, contact support at support@docketalarm.com.

Sealed Document

We are unable to display this document, it may be under a court ordered seal.

If you have proper credentials to access the file, you may proceed directly to the court's system using your government issued username and password.


Access Government Site

We are redirecting you
to a mobile optimized page.





Document Unreadable or Corrupt

Refresh this Document
Go to the Docket