`(54) RECYCLING METHOD FOR TREATING
`USED BATTERIES, IN PARTICULAR
`RECHARGEABLE BATTERIES, AND
`BATTERY PROCESSING INSTALLATION
`
`(71) Applicant: DUESENFELD GMBH, Wendeburg
`(DE)
`
`(72)
`
`Inventor: Christian Hanisch, Braunschweig (DE)
`
`(52) U.S. Cl.
`CPC ............. H0lM 10154 (2013.01); C22B 11005
`(2013.01); C22B 7100 (2013.01); C22B 71001
`(2013.01);
`
`(Continued)
`(58) Field of Classification Search
`CPC ......... H0lM 10/54; H0lM 6/52; C22B 1/005;
`C22B 7/00; C22B 7/001; Y02P 10/20;
`Y02W 30/84
`See application file for complete search history.
`
`(73) Assignee: DUESENFELD GMBH, Wendeburg
`(DE)
`
`(56)
`
`References Cited
`
`( *) Notice:
`
`Subject to any disclaimer, the term ofthis
`patent is extended or adjusted under 35
`U.S.C. 154(b) by 593 days.
`
`This patent is subject to a terminal dis(cid:173)
`claimer.
`
`(21)
`
`Appl. No.:
`
`16/343,224
`
`(22)
`
`PCT Filed:
`
`Oct. 12, 2017
`
`(86)
`
`PCT No.:
`
`PCT/EP2017/076113
`
`§ 371 (c)(l),
`(2) Date:
`
`Apr. 18, 2019
`
`(87)
`
`PCT Pub. No.: WO2018/073101
`PCT Pub. Date: Apr. 26, 2018
`
`(65)
`
`Prior Publication Data
`
`US 2019/0260101 Al
`
`Aug. 22, 2019
`
`(30)
`
`Foreign Application Priority Data
`
`Oct. 20, 2016
`
`(DE) ..................... 10 2016 120 046.8
`
`(51)
`
`Int. Cl.
`H0lM 10154
`C22B 1100
`
`(2006.01)
`(2006.01)
`(Continued)
`
`U.S. PATENT DOCUMENTS
`
`3,671,318 A
`4,118,219 A
`
`6/1972 Moe
`10/ 1978 Elmore et al.
`(Continued)
`
`FOREIGN PATENT DOCUMENTS
`
`CA
`CN
`
`11/2016
`2983768 Al
`8/2003
`1438729 A
`(Continued)
`
`OTHER PUBLICATIONS
`
`Dehnert et al: "Vacuum Distillation", Allgemeine Chemie, 14.3, p.
`14, 1979.
`
`(Continued)
`
`Primary Examiner - Stephen J Yanchuk
`(74) Attorney, Agent, or Firm - WC&F IP
`
`ABSTRACT
`(57)
`The invention relates to a method for treating used lithium
`batteries (10) containing the steps: comminuting the batter(cid:173)
`ies (10) such that comminuted material (24) is obtained, and
`(b) inactivating of the comminuted material (24) such that an
`inactive comminuted material ( 42) is obtained. According to
`the invention, the drying is conducted at a maximum pres(cid:173)
`sure of 300 hPa and a maximum temperature of 80° C. and
`the deactivated comminuted material (42) is not filled into a
`transport container and/or said deactivated comminuted
`(Continued)
`
`12
`
`32
`
`•
`
`30
`
`:
`: I
`!
`:
`:
`
`~29
`
`r;,;mlainer
`
`liqwdcleot
`
`tocomponent,;,
`
`!}-38
`oonlainer
`
`t
`
`•
`
`LI
`gasbottje
`
`50
`
`Ascend Elements EX1001 Page 1
`
`

`

`US 12,119,463 B2
`Page 2
`
`material is immediately further processed after the drying
`process.
`
`14 Claims, 4 Drawing Sheets
`
`(51)
`
`Int. Cl.
`C22B 7100
`H0JM6/52
`(52) U.S. Cl.
`CPC ............... H0JM 6152 (2013.01); Y02P 10/20
`(2015.11); Y02W 30/84 (2015.05)
`
`(2006.01)
`(2006.01)
`
`(56)
`
`References Cited
`
`U.S. PATENT DOCUMENTS
`
`CN
`DE
`DE
`DE
`DE
`DE
`DE
`EP
`EP
`EP
`EP
`JP
`JP
`JP
`JP
`JP
`JP
`JP
`JP
`JP
`JP
`JP
`JP
`KR
`KR
`KR
`WO
`WO
`WO
`WO
`WO
`
`105552470 A
`4424825 Al
`10ll8961 B4
`60 2005 001 937 T2
`10 20ll
`llO 083 Al
`10 2012 024 876 Al
`10 2015 207 843 Al
`0794587 A2
`1041659 Al
`1760821 Al
`2741357 Al
`H06338352 A
`2000243396 A
`2001012704 A
`20050ll698 A
`2005515605 A
`2005197149 A
`2007531977 A
`2008204755 A
`2013004299 A
`2013229326 A
`2015028928 A
`2016512165 A
`20040071776 A
`20060101683
`10-0665626 Bl
`2010/102377 Al
`2010/1496ll Al
`2013023640 Al
`2016/164752 Al
`2016174156 Al
`
`5/2016
`1/1996
`8/2006
`5/2008
`2/2013
`6/2014
`11/2016
`9/1997
`10/2000
`3/2007
`6/2014
`12/1994
`9/2000
`1/2001
`1/2005
`5/2005
`7 /2005
`11/2007
`9/2008
`1/2013
`11/2013
`2/2015
`4/2016
`8/2004
`3/2005
`1/2007
`9/2010
`12/2010
`2/2013
`10/2016
`11/2016
`
`OTHER PUBLICATIONS
`
`und
`Herausgeber: "Florke/WolffKursthemen Chemis-Allgemeine
`Phsyikalische Chemie", "(Course Issues Chemisty----General and
`Physical Chemistry)", 1985.
`Higgelke: "Infinite Power Solutions stellt papierdunnen Akku vor",
`"(Infinite Power Solution presents paper-thin Battery)", Jun. 6,
`2012.
`24351 Trocknungstechnik (VDMA~German Engi(cid:173)
`VDMA-Norm
`neering Federation; VDMA Standared 24351-Drying Technology(cid:173)
`Basic terms and definitions), Sep. 1999.
`Wolf et al: Allgemeine und Physikalische Chemie, Chemie, 1985.
`Carolo-Wilhelmina University of Technology in Braunschweig Final
`report "Joint project as part of the "Renewably Mobile funding
`program of the Federal Ministry for the Environment, Nature
`Conservation, Building and Nuclear Safety, Jul. 1, 2012-Mar.31,
`2016.
`Kwade, A. et al., "LithoRec Recycling von Lithium-Ionen(cid:173)
`Batterien" LithoRec, 2012.
`Perry, R. & Green, D., "Perry's Chemical Engineer's Handbook,
`Seventh Edition", 1997.
`Vacuum Technology; Terms and Definitions; General Terms. DIN
`28400-1, German Institute for Standards e.V., 1990.
`
`* cited by examiner
`
`11/1982 Goodenough
`4/1994 Milewits ................... B09B 3/00
`241/100
`
`5/1997 Meador
`9/2002 Hanisch et al.
`2/2003 Tanii et al.
`9/2006 Kiss
`3/2007 Cardarelli
`
`7/2012 Stevens
`9/2016 Dunagan et al.
`11/2016 Iida
`10/2017 Hanisch
`12/2017 Hayashi et al.
`8/2019 Shin et al.
`6/2021 Hanisch et al.
`10/2003 Sloop
`11/2005 Kakuta et al.
`9/2010 Ewles et al.
`1/2014 Iida .
`
`HOlM 6/52
`75/693
`
`HOlM 10/54
`432/13
`
`4,357,215 A
`5,303,872 A *
`
`5,632,863 A
`6,447,669 Bl
`6,524,737 Bl
`7,101,425 B2
`7,192,564 B2 *
`
`8,210,456 B2
`9,450,277 B2
`9,509,025 B2
`9,780,419 B2
`9,843,077 B2
`10,396,408 B2
`ll,050,097 B2
`2003/0186ll0 Al
`2005/0241943 Al
`2010/0230518 Al
`2014/0017621 Al*
`
`2014/0290438 Al
`2016/0043450 Al
`2016/0045841 Al*
`
`2016/0049699 Al*
`
`10/2014 Hanisch
`2/2016 Sloop
`2/2016 Kaplan
`
`2/2016 Hayashi
`
`B01D3/06
`429/49
`COlF 11/22
`44/387
`HOlM 6/52
`HOlM 10/0525
`.................... C22B47/00
`
`2016/0372802 Al*
`2018/0013181 Al*
`2018/0366740 Al*
`
`12/2016 Chiang
`1/2018 Ho
`12/2018 Muska
`
`FOREIGN PATENT DOCUMENTS
`
`CN
`CN
`CN
`CN
`
`101394015 A
`102496752 A
`103959553 A
`103259062 B
`
`3/2009
`6/2012
`7/2014
`9/2015
`
`Ascend Elements EX1001 Page 2
`
`

`

`~;ot 10.2
`jfl cr10.3
`
`,.~
`
`' discharge
`Vt'-,
`
`l
`
`~
`dismantling [~:
`
`12
`
`✓ 14
`
`'.
`
`20
`
`.c..__
`
`__
`
`__;
`
`r••••••-••••-••••••••••••·•·-•-•••
`
`16.2
`16.1~fd__
`battery modules/-cells
`~ t s.i----18
`., X ,_ __
`'
`•
`24
`•
`=J:-~as
`28 ,.rb
`.
`lcadedwith
`vofatile electrolyte:
`components
`electrolyte remo,1al
`cb-l--1'. Pw
`(under vacuum.
`,igirated.
`heating optional}
`-~
`41
`26
`I
`dried battery fr~42
`r.
`44
`
`I:!
`i
`: c&--i:xh--r"Y
`:
`!
`
`r.l
`::;,
`
`""
`"' <fl
`0 u
`0
`
`£!
`o t
`
`n
`
`L_J
`gas bottle
`
`40
`
`co~denscr
`
`32
`
`•• - ••••••
`
`/
`D
`txi
`
`----
`--__...j
`
`36
`
`30
`
`·:
`
`•
`•
`
`I
`I
`1
`
`31
`
`t-------'-----:k.J
`i
`
`dried battcrAfragm~nts
`
`l..
`! _L....----46
`~
`container
`
`l
`
`~29
`--... -. - - - - -- --- . - - . ---
`liquid electro{te componenis
`
`'
`
`38
`
`"
`'~
`I
`•
`~
`container
`
`e •
`
`00
`•
`~
`~
`~
`
`~ = ~
`
`0
`(') :-+-....
`
`"'Ul
`N
`0
`N
`.i;...
`
`('D
`
`rJJ =(cid:173)
`('D .....
`....
`0 ....
`
`.i;...
`
`d r.,;_
`"'""'
`N
`"'
`"'""'
`"'""'
`\0
`~
`
`0--, w = N
`
`so
`
`Fig. 1
`
`Ascend Elements EX1001 Page 3
`
`

`

`U.S. Patent
`
`Oct. 15, 2024
`
`Sheet 2 of 4
`
`US 12,119,463 B2
`
`44
`
`58
`
`26
`
`56
`
`18
`
`54
`
`LIi
`
`42
`
`46
`
`42
`
`Fig. 2
`
`Ascend Elements EX1001 Page 4
`
`

`

`U.S. Patent
`
`Oct. 15, 2024
`
`Sheet 3 of 4
`
`US 12,119,463 B2
`
`88
`
`80
`
`76
`
`62
`
`68
`
`86
`
`78
`
`72
`
`42
`
`Fig. 3
`
`Ascend Elements EX1001 Page 5
`
`

`

`U.S. Patent
`
`Oct. 15, 2024
`
`Sheet 4 of 4
`
`US 12,119,463 B2
`
`10.1
`
`~ 11 °"--10.2
`
`22
`
`~12
`~ ----._.14
`161-:-°l
`~16.2
`27 "-U}J
`x-----'-------a:-~--~
`
`____,,~-----.-~
`_/i
`: 42 --------
`----------l-
`42
`,-c~ ~ ~-
`
`-I
`I
`I
`30 :
`:
`
`---~..!
`----------~29
`
`38
`
`98
`
`52 I
`
`94
`
`50
`
`r
`
`110
`
`62
`
`_,--+~------ ►
`
`:
`
`n-!~-~-----J
`
`..... \___88.4
`
`Fig. 4
`
`Ascend Elements EX1001 Page 6
`
`

`

`US 12,119,463 B2
`
`1
`RECYCLING METHOD FOR TREATING
`USED BATTERIES, IN PARTICULAR
`RECHARGEABLE BATTERIES, AND
`BATTERY PROCESSING INSTALLATION
`
`2
`installation is connected to the drying device in order to
`generate a vacuum of at least 300 hPa in the drying device,
`and the drying device is configured to dry at a maximum
`temperature of 80° C.
`The advantage of the invention is that the amount of
`electrolyte that can be obtained from the comminuted mate(cid:173)
`rial through drying is such that an electrochemical reaction
`is no longer possible, or only to a negligibly small extent. In
`addition, no flammable or explosive gas phase forms above
`10 the battery fragments, as the organic carbonates of the
`electrolyte that have a low boiling point have been removed
`[from the fragments]. The comminuted material is therefore
`largely inert and can be safely transported or processed
`further, especially if it is packed under vacuum.
`A further advantage is that no additional material has to be
`added to deactivate the comminuted material. This decreases
`the complexity of the battery processing, reduces the weight
`of the deactivated comminuted material and increases the
`purity in the subsequent separation and recycling steps. In
`particular, in potential subsequent hydrometallurgical pro(cid:173)
`cessing steps, a high degree of product purity without
`foreign ions is advantageous.
`It is also advantageous that the formation of relevant
`quantities of fluorophosphates, hydrogen fluoride, carbon
`monoxide, polyfluorinated dibenzodioxins and dibenzo(cid:173)
`furans, nitrogen oxides, carbonyl fluoride and/or hydrogen
`cyanide can be ruled out. Fluorophosphates are often strong
`neurotoxins, the formation of which must be reliably pre(cid:173)
`vented. Furthermore, due to the low electrolyte content, it is
`guaranteed that a self-amplifying and intensifying build-up
`of heat triggered by an electrochemical reaction cannot
`occur. It has been proven that hydrogen fluoride and fluo(cid:173)
`rophoshate can form in significant quantities at compara(cid:173)
`tively low temperatures of over 80° C.
`Furthermore, it is advantageous that the removal of the
`electrolyte is possible without expending a considerable
`amount of energy. The electrolyte can also be largely reused.
`The condensation of the vaporised electrolyte, as intended
`according to a preferred embodiment, also leads to a low-
`40 emission recycling of lithium batteries.
`The battery processing installation according to the inven(cid:173)
`tion enables material recycling rates of over 80%, which is
`not possible with current installations.
`Within the scope of the present description, the term
`45 drying should be understood particularly
`to mean the
`removal of at least one solvent in the conducting salt. In
`particular, the drying is executed such that at least 90 percent
`by weight of dimethyl carbonate and/or ethyl methyl car(cid:173)
`bonate is removed.
`A lithium battery should to understood particularly to
`mean a rechargeable battery whose electrochemical reaction
`involves lithium and/or lithium ions and/or a lithium com(cid:173)
`pound.
`A battery processing installation should also be under-
`55 stood particularly to mean a rechargeable battery processing
`installation for processing rechargeable batteries.
`The transport container should also be understood par(cid:173)
`ticularly to mean transport packaging. The transport pack(cid:173)
`aging is preferably sealed by way of a vacuum seal. Alu-
`60 minium composite foil is especially well-suited as transport
`packaging.
`The comminution unit should be understood especially to
`mean a device which, when operating, comminutes the
`batteries. For example, the comminution unit (i) is a pressure
`65 comminution unit whereby the batteries are crushed between
`two tool surfaces, (ii) a striking comminution unit whereby
`the batteries lie on a tool surface and are smashed by striking
`
`25
`
`The invention refers to a method for the treatment of used
`batteries, in particular used lithium batteries, such as lithium
`ion batteries, with the steps (a) comminuting the batteries
`such that comminuted material is obtained, (b) inactivating
`of the comminuted material such that an inactive commi(cid:173)
`nuted material is obtained.
`According to a second aspect, the invention refers to a
`battery processing installation for the treatment of used
`batteries, in particular for the treatment of used lithium
`batteries with (a) a comminuting device for comminuting the 15
`batteries such that comminuted material is obtained, and (b)
`an inactivation device for inactivating the comminuted
`material.
`US 2005/0241943 Al describes a method for processing
`used batteries in which the batteries are heated prior to a 20
`comminuting step, thereby destroying plastic components in
`the batteries. The disadvantage of this type of procedure is
`that the remaining components of the batteries may be
`contaminated with degradation products of the plastic.
`DE 10 2012 024 876 Al describes a system for transfer-
`ring transport-critical electrolyte cells, in which they are
`initially comminuted under inert gas and then dusted with a
`deactivation powder so as to prevent the electrochemically
`active material from spontaneously combusting. The disad(cid:173)
`vantage of this is that the resulting material still poses a 30
`comparatively high hazard potential and that the dusting
`power itself poses a risk of exposure and that the formation
`of a flammable and explosive atmosphere in the transport
`container cannot be ruled out.
`DE 10 2011 110 083 Al describes a method for recov-
`ering active material from a galvanic cell, in which the
`galvanic cells are initially mechanically comminuted, then
`pre-dried and subsequently sifted. Finally, the binder is
`broken down in an oven.
`This type of device is very well-suited to the efficient
`recycling of larger amounts of galvanic elements. However,
`for partial load operation, the construction of this installation
`is comparatively complex. It has also been proven that
`highly toxic fluoroorganic compounds and hydrogen fluo(cid:173)
`ride may form, the disposal of which is highly complex.
`WO 2010/102377 Al describes a method in which the
`batteries to be recycled, such as lithium batteries, are heated
`in a rotary kiln and the resulting gases are sucked away. The
`disadvantage of this method is that it is difficult to reuse the
`electrolyte and it produces large quantities of hydrogen 50
`fluoride and fluoro-organic compounds.
`The post-published publication WO 2016/174156 Al
`describes a method in which used batteries are first locally
`deactivated and placed in a transport container. Following
`the transport of the comminuted material to a central pro(cid:173)
`cessing plant, the deactivated cell fragments are processed
`further.
`The invention aims to reduce disadvantages of the prior
`art.
`The invention solves the problem by way of a method
`according to the preamble in which the drying is conducted
`at a maximum pressure of 300 hPa, preferably at least in part
`at 50 hPa, and at a maximum of 80° C. In particular, the
`deactivation is conducted at least also by drying the com(cid:173)
`minuted material. According to a second aspect, the inven(cid:173)
`tion solves the problem by way of a battery processing
`installation according to the preamble, wherein a vacuum
`
`35
`
`Ascend Elements EX1001 Page 7
`
`

`

`US 12,119,463 B2
`
`5
`
`3
`them with a second moveable tool, (iii) a cropping commi(cid:173)
`nution unit whereby the batteries are comminuted by two
`tool surfaces that move in opposite directions, (iv) a cutting
`comminution unit whereby the batteries are cut into two
`parts by means of two blades and/or (v) an impact commi-
`nution whereby the batteries are thrown against a wall,
`impact against a moving tool or two particles collide. Of
`course, the comminution unit may also work by way of two
`or more of the named comminution mechanisms.
`According to a preferred embodiment, the comminution 10
`unit forms part of a comminuting device which comprises a
`container in which the comminution unit is arranged.
`The given temperatures and pressures always relate to the
`atmospheric temperature in the respective device. In this
`way, the characteristic that the drying occurs at a maximum 15
`pressure of 300 hPa and at a maximum of 80° C. should be
`understood particularly to mean that the temperature of the
`atmosphere in the dryer is a maximum of 80° C. It is
`irrelevant that the local temperature may be higher.
`It is beneficial if the drying occurs after the comminuting 20
`of the batteries. It is indeed possible and represents a
`preferred embodiment that the batteries are exposed to a
`vacuum when in an uncomminuted state such that at least
`parts of the electrolyte vaporise, wherein the resulting gas
`either escapes through a safety valve in the rechargeable 25
`battery or the battery is destroyed by the pressure difference
`between the external environment and the internal pressure,
`enabling the vaporising electrolyte to escape. However,
`since the electrolyte
`is predominantly
`located between
`tightly wound or stacked and pressed layers of electrodes 30
`and separators and in their pores, and it is connected to other
`components of the batteries, this procedure can be very
`time-consuming. It is thus often more beneficial and repre(cid:173)
`sents a preferred embodiment of the invention for the
`batteries to be mechanically comminuted, for example 35
`through cutting, cropping, impact, cutting and/or crushing.
`This means that a larger interface is available for the
`transition of materials into the gas phase.
`The drying process is preferably conducted at a maximum
`pressure of 30 hPa for at least 50% of the drying time. 40
`Alternatively or additionally, a minimum pressure during the
`drying process is at most 50 hPa. This allows for the removal
`of a very large proportion of the electrolyte. The minimum
`pressure should be understood especially to mean the lowest
`atmospheric pressure in the drying device that is maintained 45
`for at least one minute.
`According to a preferred embodiment, it is also possible
`for the drying to occur at the same time as the comminuting.
`In other words, a vacuum with a maximum pressure of 300
`hPa is attached to a comminuting device in which the 50
`batteries are comminuted. The advantage of this is that the
`mechanical energy introduced during comminuting supports
`the vaporising of the electrolyte. It is therefore not necessary
`to introduce additional thermal energy into the comminuted
`material in order to vaporise the electrolyte (although this is 55
`possible and included in the invention). Furthermore, it is
`not necessary to cool the comminuted material during com(cid:173)
`minuting (although this is possible and included in the
`invention). The comminution unit also effects a circulation
`of the comminuted material, which accelerates the drying 60
`process.
`It is favourable if the drying occurs while the comminuted
`material is being agitated and/or circulated. This results in
`the separation of the galvanic elements, which consist of
`anode, separator and cathode. An obstruction of the vaporis(cid:173)
`ing process by way of foils which stick together is pre(cid:173)
`vented. Mechanical energy is introduced for the separation
`
`4
`of current collector foil and coating, and the resulting
`frictional heat feeds the vaporising heat into the system.
`Prior to being comminuted, the used batteries are prefer(cid:173)
`ably dismantled. This means that larger battery systems are
`dismantled into their smaller subcomponents, the modules
`or stacks, or even that the cells which contain the electro-
`chemically active material are separated from the control
`electronics. The control electronics comprise, for example,
`semiconductor elements and/or sensors and are responsible
`for the charge control of the batteries.
`The drying occurs under a vacuum. According to its most
`general configuration, the invention solves the problem by
`means of a method according to the preamble, wherein the
`vacuum is selected to be so large that the pressure is below
`the vapour pressure of dimethyl carbonate at 80° C., in
`particular at 70° C. However, it is especially beneficial if the
`drying occurs at a maximum pressure of 300 hPa, in
`particular a maximum of 100 hPa. At such low pressures,
`considerable parts of most electrolytes vaporise, especially
`dimethyl carbonate and ethyl methyl carbonate, and do so at
`temperatures of less than 80° C. The advantage of low
`temperatures is that the formation of hydrogen fluoride and
`fluoro-organic compounds is hindered. Both pose a potential
`risk for the battery processing installation and the surround(cid:173)
`ings. It is therefore beneficial to prevent their development.
`The drying preferably occurs at a temperature that is
`lower than a decomposition temperature. The decomposition
`temperature should be understood particularly to mean the
`lowest temperature at which at least 80 percent by mass of
`the binder of the lithium batteries has decomposed into
`gaseous components after keeping the comminuted material
`at this temperature for an hour. The decomposition tempera(cid:173)
`ture can be measured by successively increasing the tem(cid:173)
`perature of the comminuted material and recording when a
`loss of mass occurs, especially through the build-up of gas
`due to a decomposition of the binder, and the specified
`criteria is fulfilled. If necessary, the experiment must be
`conducted several times, each time using a new sample of
`comminuted material at an increased temperature.
`According to a preferred embodiment, the method com(cid:173)
`prises the condensation of the gases which result from the
`drying process. This preferably occurs at ambient pressure,
`whereby a deviation of ±50 hPa is possible. It is beneficial
`if the temperature during condensation is at least 0° C. This
`reduces the required cooling capacity and prevents the
`formation of ice. The cooling capacity is preferably at least
`4 kilowatts and at most 40 kilowatts relative to one tonne of
`processed batteries per hour. Alternatively, the temperature
`upon condensation is lower than 0° C., such that water is
`removed from the atmosphere through the formation of ice.
`It is possible that the condenser has two or more zones of
`varying temperature. In this case, the temperature in one of
`the two zones is so high that no ice forms and so low in
`another zone that water is separated as ice.
`It is favourable if the maximum temperature upon con(cid:173)
`densation is at most 50° C., preferably a maximum of30° C.,
`in particular a maximum of 20° C. This means that the
`organic carbonates in the batteries can be almost completely
`recovered. Moreover, virtually no emissions are produced
`and the amount of energy required for condensation is low.
`The comminuting of the batteries is preferably executed
`such that at least 90% by weight of the components of the
`comminuted material has a maximum sieve size of 50 mm,
`in particular a maximum of 30 mm, preferably a maximum
`65 of 20 mm. This should be understood to mean that 90% by
`weight of the components fall through a sieve which has a
`mesh width of 50 mm (or the respective given width). This
`
`Ascend Elements EX1001 Page 8
`
`

`

`US 12,119,463 B2
`
`5
`type of comminuting avoids micro short circuits, thereby
`increasing the level of safety of transport, storage and further
`processing.
`It is favourable if the drying occurs under an atmosphere
`in which the partial pressure of the water is lower than 50 Pa,
`in particular lower than 10 Pa. A low partial pressure of the
`water leads to a low reaction rate of lithium compounds to
`lithium hydroxide and thus only to a low build-up of
`hydrogen. This prevents the formation of flammable hydro(cid:173)
`gen-oxygen mixtures and contributes to the safety of the
`installation.
`In addition, it is favourable if the partial pressure of
`oxygen upon drying has a maximum value of 30 millibars,
`especially a maximum value of 10 millibars. This largely
`inhibits the reaction of oxygen with oxidisable components
`of the batteries. It is possible to achieve the low partial
`pressure of oxygen by means of drying at a low pressure.
`Alternatively or additionally, the drying may occur in an
`inert gas atmosphere.
`According to a preferred embodiment, the method com(cid:173)
`prises the steps of a continuous recording of a water vapour
`concentration during comminuting and/or drying, and a
`reduction of the water vapour concentration when a pre(cid:173)
`determined threshold value is exceeded. The water vapour
`concentration should be understood especially to mean a
`proportion of water vapour in relation to the entirety of the
`atmospheric components. In particular, the water vapour
`concentration should also be understood to mean a partial
`water vapour pressure. For instance, the reduction of the
`water vapour concentration may comprise a decrease in the
`pressure and/or a supply of inert gas. The threshold value for
`the water vapour concentration is preferably selected such
`that, below the threshold value, a formation of significant
`quantities of hydrogen fluoride through decomposition of
`the conducting salt, such as LiPF 6 , and a significant reaction
`of the water with metallic lithium is impossible. These
`criteria are met at a dew point of -40° C. It is possible, but
`not necessary, for the water vapour concentration to be
`measured directly, for instance by spectroscopy, especially
`infrared spectroscopy. It is also possible, for example, to
`identify the sum of the concentrations of inert gas, oxygen
`and organic compounds and assume that the rest is made up
`of water vapour.
`According to a preferred embodiment, the method com(cid:173)
`prises the steps of a continuous recording of a oxygen
`concentration during comminuting and/or drying, and a
`reduction of the oxygen concentration when a pre-deter(cid:173)
`mined threshold value is exceeded. The oxygen concentra(cid:173)
`tion should be understood especially to mean a proportion of
`oxygen in relation to the entirety of the atmospheric com(cid:173)
`ponents. In particular, the oxygen concentration should also
`be understood to mean a partial oxygen pressure. The
`reduction of the oxygen concentration may comprise, for
`example, a decrease in the pressure and/or a supply of inert
`gas. The threshold value for the oxygen concentration is
`preferably selected such that an explosion is impossible
`below the threshold value. It is possible, but not necessary,
`for the oxygen concentration to be measured directly, for
`instance using a Nernst probe, a lambda probe, paramagnetic
`sensors or a resistive probe. It is also possible, for example,
`to determine the concentration of the oxygen by measuring
`gases in air that are accompanied by oxygen, such as carbon
`dioxide by assuming that the same mixing ratio of oxygen is
`present in the measured gas as in the air.
`In particular, the method comprises the steps (i) continu(cid:173)
`ous monitoring of a concentration of organic carbonates in
`the atmosphere of the drying device during drying and (ii)
`
`6
`completion of the drying when a lower explosion limit is no
`longer reached. The lower explosion limit is the concentra(cid:173)
`tion of organic components for which the following applies:
`following the filling of a container with the comminuted
`5 material in air with a temperature of 23° C., under 1013 hPa
`and at 80% humidity, an ignition does not cause an explo(cid:173)
`sion but does lead to a higher concentration. If this lower
`explosion limit is still reached, the drying continues.
`The concentration of inert gas is preferably set at at least
`10 90% by weight, in particular at least 95% by weight,
`preferably at least 97% by weight. The measurement of the
`concentration is preferably done, for example, spectroscopi(cid:173)
`cally.
`Alternatively or additionally, a progress parameter is
`15 recorded which describes the progress of the drying, and the
`drying is completed when the progress parameter reaches a
`pre-determined progress parameter threshold value. The
`progress parameter is small at the beginning of the drying
`and increases with the progression of the drying. An equiva-
`20 lent situation is for the progress parameter to be large at the
`beginning of the drying and to decrease with the progression
`of the drying.
`For instance, the progress parameter is the concentration
`of a gaseous electrolyte in the gas which has been sucked
`25 out. In this situation, it is possible, but not necessary, to
`directly measure the concentration of a gaseous electrolyte,
`in particular organic carbonates, for instance by spectros(cid:173)
`copy, especially infrared spectroscopy. Alternatively or addi(cid:173)
`tionally, it is possible that the progress parameter is the
`30 condensate flow (measured, for example, in volume, mass,
`weight or quantity of substance per time unit) of condensed
`gas components in an available condenser. Alternatively, the
`progress parameter is the pressure in the drying container or
`the gas flow out of the drying container. If a pump output is
`35 constant, the pressure only depends, in good approximation,
`on the drying progress and the temperature of the commu(cid:173)
`nited material. If the electrolyte has largely been vaporised,
`the pressure decreases. The gas flow also reduces.
`According to a preferred embodiment, the comminuted
`40 material is further processed immediately after the drying
`process. In particular, the comminuted material is not put in
`a transport container after drying. In particular, the commi(cid:173)
`nuted material is transported after drying by means of a
`continuously or discontinuously feeding conveyor for fur-
`45 ther processing, for example a separating device. In particu(cid:173)
`lar, the conveyor is connected to the dryer such that it is
`dust-tight. Examples of a continuously feeding conveyor are
`dust-tight tube chain conveyors, preferably with two adjust(cid:173)
`able outlet slides, conveyors, conveyor troughs, screw con-
`50 veyors, bucket conveyors or semi-continuous conveyors.
`A method is preferred in which the drying of the com(cid:173)
`minuted material is only completed if, after the completion
`of the drying process, no flammable or explosive gas mix(cid:173)
`ture can form above the comminuted material that has been
`55 filled [in the container] and/or when the comminuted mate(cid:173)
`rial is so dry that no flanimable or explosive gas mixture can
`emerge in the transport container or during the subsequent
`processing. The property that the drying is completed if,
`after the completion of the drying process, no flammable or
`60 explosive gas mixture can form above the comminuted
`material that has been filled [in the container] should be
`understood particularly to mean that, within the space of one
`week at 50° C. and 1013 hPa, no flanimable gas mixture
`forms in a transport container in the form of a 50 litre
`65 container that has been half-filled (relative to its volume)
`with the comminuted material. Preliminary tests determine
`whether the criteria has been fulfilled. If a flammable gas
`
`Ascend Elements EX1001 Page 9
`
`

`

`US 12,119,463 B2
`
`15
`
`7
`mixture does form, the drying must be conducted for a
`longer time and/or at a lower pressure. The preliminary tests
`are repeated until a drying time and/or drying pressure has
`been identified at which, in a set of tests of three transport
`containers, the requirements for the property have been
`fulfilled for all three transport containers.
`The comminuted material is preferably dried until an
`electrolyte content in the comminuted material is so low that
`an electrochemical reaction is impossible. In other words,
`the electrolyte content is lower than a threshold value, the 10
`threshold value being selected such that, if this threshold
`value is not achieved, the cell voltage is reduced to a
`maximum of one quarter. This threshold value is deter(cid:173)
`mined, for example, by defining the cell voltage of a battery
`in relation to the electrolyte content. Shortly before achiev-
`ing the threshold value, the cell voltage collapses, i.e. it
`decreases by at least 75%. If the threshold value is not
`achieved, the battery contains so little electrolyte that, to a
`good approximation, an electrochemical reaction is no lon(cid:173)
`ger possible.
`The comminuted material is preferably dried for so long
`that a 50 kg amount of comminuted material, which is
`contained in a compacted form in a 50 litre drum, does not
`experience a build-up of heat, or the build-up of heat is so
`lo

This document is available on Docket Alarm but you must sign up to view it.


Or .

Accessing this document will incur an additional charge of $.

After purchase, you can access this document again without charge.

Accept $ Charge
throbber

Still Working On It

This document is taking longer than usual to download. This can happen if we need to contact the court directly to obtain the document and their servers are running slowly.

Give it another minute or two to complete, and then try the refresh button.

throbber

A few More Minutes ... Still Working

It can take up to 5 minutes for us to download a document if the court servers are running slowly.

Thank you for your continued patience.

This document could not be displayed.

We could not find this document within its docket. Please go back to the docket page and check the link. If that does not work, go back to the docket and refresh it to pull the newest information.

Your account does not support viewing this document.

You need a Paid Account to view this document. Click here to change your account type.

Your account does not support viewing this document.

Set your membership status to view this document.

With a Docket Alarm membership, you'll get a whole lot more, including:

  • Up-to-date information for this case.
  • Email alerts whenever there is an update.
  • Full text search for other cases.
  • Get email alerts whenever a new case matches your search.

Become a Member

One Moment Please

The filing “” is large (MB) and is being downloaded.

Please refresh this page in a few minutes to see if the filing has been downloaded. The filing will also be emailed to you when the download completes.

Your document is on its way!

If you do not receive the document in five minutes, contact support at support@docketalarm.com.

Sealed Document

We are unable to display this document, it may be under a court ordered seal.

If you have proper credentials to access the file, you may proceed directly to the court's system using your government issued username and password.


Access Government Site

We are redirecting you
to a mobile optimized page.





Document Unreadable or Corrupt

Refresh this Document
Go to the Docket

We are unable to display this document.

Refresh this Document
Go to the Docket